Àá½Ã¸¸ ±â´Ù·Á ÁÖ¼¼¿ä. ·ÎµùÁßÀÔ´Ï´Ù.

µµÀç¶ó¹Ì³×ÀÌÆ® Á¢Âø¿ë ·¹Áø½Ã¸àÆ®ÀÇ »öÁ¶ ¾ÈÁ¤¼º¿¡ °üÇÑ ¿¬±¸

A STUDY ON THE COLOR STABILITY OF RESIN CEMENTS LUTED FOR PORCELAIN LAMINATE VENEER

´ëÇÑÄ¡°úº¸Ã¶ÇÐȸÁö 2007³â 45±Ç 2È£ p.191 ~ 202
±è¿µ¿î, ¹Ú»ó¿ø, ¾çÈ«¼Ò, ¹æ¸ù¼÷, ¹ÚÇÏ¿Á,
¼Ò¼Ó »ó¼¼Á¤º¸
±è¿µ¿î ( Kim YOung-Woon ) - Àü³²´ëÇб³ Ä¡ÀÇÇÐÀü¹®´ëÇпø Ä¡°úº¸Ã¶Çб³½Ç
¹Ú»ó¿ø ( Park Sang-Won ) - Àü³²´ëÇб³ Ä¡ÀÇÇÐÀü¹®´ëÇпø Ä¡°úº¸Ã¶Çб³½Ç
¾çÈ«¼Ò ( Yang Hong-So ) - Àü³²´ëÇб³ Ä¡ÀÇÇÐÀü¹®´ëÇпø Ä¡°úº¸Ã¶Çб³½Ç
¹æ¸ù¼÷ ( Vang Mong-Sook ) - Àü³²´ëÇб³ Ä¡ÀÇÇÐÀü¹®´ëÇпø Ä¡°úº¸Ã¶Çб³½Ç
¹ÚÇÏ¿Á ( Park Ha-Ok ) - Àü³²´ëÇб³ Ä¡ÀÇÇÐÀü¹®´ëÇпø Ä¡°úº¸Ã¶Çб³½Ç

Abstract


Statement of problems: Long-term success of esthetic restorations, depends on various factors, especially on color stability of the restorations. The color stability is affected by resin cements beneath the porcelain laminate veneers.

Purpose: The purpose of this study was to comprehend the color stability of resin cements by comparing with 4 different kinds of resin cements (Choice, Variolink II, Nexus 2, Rely-X).

Material and methods: Porcelain laminate disk samples were luted with resin cements. After thermocycling of each 1000, 2000 and 3000 cycle, specimens were measured by spectrophotometers and the color differences were.

Results: 1. After thermocycling of 1000, 2000 and 3000cycle, color difference, ({Delta}E^*) of all specimens were incresed, but were not statiscally significant differences. 2. In the Choice of A1 shade and the Nexus 2 of A3 shade, color difference({Delta}E^*) after thermocycling of 3000cycle was incre^*ased significantly than after thermocycling of 1000cycle. However, other groups did not show any statistically significant differences (P<0.05). 3. After thermocycling of 3000cycle, color difference({Delta}E^*)between A1 shade and A3 shade of Nexus 2 showed statistically significant difference. However no statistically significant differences were observed in other groups (P<0.05). 4. The mean of color difference({Delta}E^*) is 1.0-2.06 after 3000 thermocycling and the data were ranked in the ascending order of Variolink II, Nexus 2, Choice and Rely-X in A1 shade group and Choice, Rely-X, Variolink II and Nexus 2 in A3 shade group.

Conclusion: Above results revealed that, after 3000 thermocycing, the color difference ({Delta}E^*) of experimental resin cements was within clinically acceptable ranges. Color stability of 4 different resin cements was comparatively excellent.

Å°¿öµå

Color stability;Resin cement;Porcelain laminate veneer;Thermocycling